NB/SH/T 0877-2014 The evaluation of oil一elastomer compatibility
WARNING: The application of this standard may involve hazardous materials, operations and equipment. This standard does not purport to address all of the safety problems associated with its use. It is the responsibility of the user of this standard to establish appropriate safety and health practices and to determine the applicability of regulatory limitations prior to use.
1 Scope
This standard specifies a method for testing the compatibility of automotive lubricating oils with vulcanized rubbers using four standard rubbers: fluororubber (RE1), polyacrylate rubber (RE2-99), silicone rubber (RE3-04) or acrylonitrile-butadiene rubber (RE4).
This standard is applicable to the determination of the compatibility of automotive lubricating oils with vulcanized rubbers.
2 Normative references
The following referenced documents are indispensable for the application of this document. For dated references, only the edition cited applies. For undated references,the latest edition of the referenced document (including any amendments) applies.
GB/T 528—2009 Rubber, vulcanized or thermoplastic — Determination of tensile stress-strain properties (10-100IRHD) (ISO 37:2005 IDT)
GB/T 531.1 Rubber vulcanized or thermoplastic — Determination of indentation hardness — Part 1: Duromerer method (Shore hardness) (GB/T 531.1—2008, ISO 7619-1:2004 IDT)
GB/T 1690 Rubber, vulcanized or thermoplastic — Determination of the effect of liquids (GB/T 1690—2006, ISO 1817: 2005)
GB/T 6031 Rubber, vulcanized or thermoplastic — Determination of hardness (GB/T 6031-1998, ISO 48:1994)
GB/T 6682—2008 Water for analytical laboratory use — Specification and test methods (ISO 3696:1987, MOD)
3 Terms and definitions
For the purposes of this document, the following terms and definitions apply.
3.1
tensile stress S
stress produced in the test sample when it is stretched, equal to the applied force divided by the original cross-sectional area of the test sample
3.2
elongation percent E
deformation of the test sample caused by the tensile stress; the value is called elongation percent and is expressed as a percentage of the ratio of the elongation increment to the original length
3.3
elongation at break EAB
elongation percent of the test sample at the moment of rupture
3.4
tensile strength TS
maximum tensile stress in the process of stretching the test sample to fracture
3.5
tensile strength at break TSB
tensile stress recorded at the moment of rupture of the stretched test sample
4 Method summary
Dumb-bell-shaped test pieces are cut from the specified rubber sheets and immersed in the test oil at the specified temperature for a specified period of time; the tensile properties, hardness and volume of the test pieces before and after immersion are measured, and the elastomer compatibility is characterized by the changes in the properties of the rubber pieces before and after immersion in the oil.
5 Apparatus
5.1 Cutting die and cutting machine: a cutting die and cutting machine capable of cutting the Type 2 test pieces specified in GB/T 528—2009.
5.2 Test piece punch.
5.3 Micro thickness gauge: with an accuracy of 0.01 mm.
5.4 Hardness tester: a micro IRHD hardness tester conforming to GB/T 6031 or a Shore A hardness tester conforming to GB/T 531.1 may be used.
NOTE In case of dispute over the test results, the results measured with the micro IRHD hardness tester shall prevail.
5.5 Electronic balance: capable of weighing up to 270 g, with an accuracy of 0.01 g.
5.6 Beaker: a lipless glass beaker with a capacity of about 400 mL, shown in Figure 1.
5.7 Glass beaker cover and holder: a glass beaker cover and holder that ensure the dumb-bell-shaped test pieces are immersed in the test oil without touching the walls of the beaker. All sides of each test piece shall be immersed in the test oil, and the test pieces shall not touch one another. See Figure 1.
5.8 Oven: with temperature control capability at 150 °C±2 °C and 100 °C±2 °C.
5.9 Tensile testing machine: a tensile testing machine with an extensometer, conforming to GB/T 528—2009.
Figure 1 Beaker and holder
6 Reagents and materials
6.1 Reagents
6.1.1 n-Heptane: analytical reagent grade.
6.1.2 Water: meeting the requirements of grade 3 water specified in GB/T 6682—2008.
6.2 Materials
6.2.1 Rubbers:
6.2.1.1 The four standard rubbers used in this standard are listed in Table 1.
Foreword II
1 Scope
2 Normative references
3 Terms and definitions
4 Method summary
5 Apparatus
6 Reagents and materials
7 Calibration of apparatus
8 Reference oils
9 Preparation of test pieces
10 Test procedure
11 Calculation of results
12 Result report
13 Accuracy and deviation
Annex A (Informative) Comparison between this standard and CEC L-39-T-96 (2011) in clause number
Annex B (Informative) Reference oils and accuracy statement
NB/SH/T 0877-2014 The evaluation of oil一elastomer compatibility
WARNING: The application of this standard may involve hazardous materials, operations and equipment. This standard does not purport to address all of the safety problems associated with its use. It is the responsibility of the user of this standard to establish appropriate safety and health practices and to determine the applicability of regulatory limitations prior to use.
1 Scope
This standard specifies a method for testing the compatibility of automotive lubricating oils with vulcanized rubbers using four standard rubbers: fluororubber (RE1), polyacrylate rubber (RE2-99), silicone rubber (RE3-04) or acrylonitrile-butadiene rubber (RE4).
This standard is applicable to the determination of the compatibility of automotive lubricating oils with vulcanized rubbers.
2 Normative references
The following referenced documents are indispensable for the application of this document. For dated references, only the edition cited applies. For undated references,the latest edition of the referenced document (including any amendments) applies.
GB/T 528—2009 Rubber, vulcanized or thermoplastic — Determination of tensile stress-strain properties (10-100IRHD) (ISO 37:2005 IDT)
GB/T 531.1 Rubber vulcanized or thermoplastic — Determination of indentation hardness — Part 1: Duromerer method (Shore hardness) (GB/T 531.1—2008, ISO 7619-1:2004 IDT)
GB/T 1690 Rubber, vulcanized or thermoplastic — Determination of the effect of liquids (GB/T 1690—2006, ISO 1817: 2005)
GB/T 6031 Rubber, vulcanized or thermoplastic — Determination of hardness (GB/T 6031-1998, ISO 48:1994)
GB/T 6682—2008 Water for analytical laboratory use — Specification and test methods (ISO 3696:1987, MOD)
3 Terms and definitions
For the purposes of this document, the following terms and definitions apply.
3.1
tensile stress S
stress produced in the test sample when it is stretched, equal to the applied force divided by the original cross-sectional area of the test sample
3.2
elongation percent E
deformation of the test sample caused by the tensile stress; the value is called elongation percent and is expressed as a percentage of the ratio of the elongation increment to the original length
3.3
elongation at break EAB
elongation percent of the test sample at the moment of rupture
3.4
tensile strength TS
maximum tensile stress in the process of stretching the test sample to fracture
3.5
tensile strength at break TSB
tensile stress recorded at the moment of rupture of the stretched test sample
4 Method summary
Dumb-bell-shaped test pieces are cut from the specified rubber sheets and immersed in the test oil at the specified temperature for a specified period of time; the tensile properties, hardness and volume of the test pieces before and after immersion are measured, and the elastomer compatibility is characterized by the changes in the properties of the rubber pieces before and after immersion in the oil.
5 Apparatus
5.1 Cutting die and cutting machine: a cutting die and cutting machine capable of cutting the Type 2 test pieces specified in GB/T 528—2009.
5.2 Test piece punch.
5.3 Micro thickness gauge: with an accuracy of 0.01 mm.
5.4 Hardness tester: a micro IRHD hardness tester conforming to GB/T 6031 or a Shore A hardness tester conforming to GB/T 531.1 may be used.
NOTE In case of dispute over the test results, the results measured with the micro IRHD hardness tester shall prevail.
5.5 Electronic balance: capable of weighing up to 270 g, with an accuracy of 0.01 g.
5.6 Beaker: a lipless glass beaker with a capacity of about 400 mL, shown in Figure 1.
5.7 Glass beaker cover and holder: a glass beaker cover and holder that ensure the dumb-bell-shaped test pieces are immersed in the test oil without touching the walls of the beaker. All sides of each test piece shall be immersed in the test oil, and the test pieces shall not touch one another. See Figure 1.
5.8 Oven: with temperature control capability at 150 °C±2 °C and 100 °C±2 °C.
5.9 Tensile testing machine: a tensile testing machine with an extensometer, conforming to GB/T 528—2009.
Figure 1 Beaker and holder
6 Reagents and materials
6.1 Reagents
6.1.1 n-Heptane: analytical reagent grade.
6.1.2 Water: meeting the requirements of grade 3 water specified in GB/T 6682—2008.
6.2 Materials
6.2.1 Rubbers:
6.2.1.1 The four standard rubbers used in this standard are listed in Table 1.
Contents of NB/SH/T 0877-2014
Foreword II
1 Scope
2 Normative references
3 Terms and definitions
4 Method summary
5 Apparatus
6 Reagents and materials
7 Calibration of apparatus
8 Reference oils
9 Preparation of test pieces
10 Test procedure
11 Calculation of results
12 Result report
13 Accuracy and deviation
Annex A (Informative) Comparison between this standard and CEC L-39-T-96 (2011) in clause number
Annex B (Informative) Reference oils and accuracy statement